Most metal-oxide surge arresters that fail in service fail from one of five causes, and four of them leave evidence you can read before the unit is cut open. A ruptured housing points to discharge energy or internal pressure; a low DC reference voltage on a unit that still looks intact usually means moisture ingress or ageing, not a lightning strike. The tests that separate the two are cheap and can be run on site.

Why Do Surge Arresters Fail Before Their Rated Life?

An arrester is sacrificial in a way a circuit breaker is not. It is expected to absorb discharge energy and then sit at full system voltage for years between events, so its service life is set by the duty it sees and by the environment around it, not by a calendar figure on the datasheet.

Five mechanisms account for most field failures in 3–220 kV work. They differ in what the teardown shows, what the field test reads, and whether the correct response is one replacement or a decision about the whole batch.

Failure modeWhat the teardown showsField evidence that points to itFirst action
Moisture ingress through a sealTracking paths and white deposits on the block column, corroded spring contacts, water in the cavity, a split starting at a shed root or at an end fittingInsulation resistance far below the commissioning record; U1mA lower than recorded; resistive leakage higherQuarantine the unit, test the neighbours, review the sealing procedure used at installation
Continuous power-frequency overvoltageUniform overheating across the whole block column, glazed or cracked blocks, a circumferential split, no single puncture pointFault coincides with an earth fault, a ferroresonant condition, or a system whose earthing arrangement differs from the one specifiedCheck the continuous operating voltage against the real maximum phase-to-earth voltage
Energy beyond the class ratingOne puncture hole or a small cluster of fragmented blocks, metal spray confined to one area, a radial splitCounter advanced sharply after a storm; exposed line, long leads, shielded conductor with no line arresterReview the discharge class and the installation position, not only the failed unit
Varistor ageing and thermal runawayLittle visible damage; slightly discoloured block faces; a burnt spot where a block meets its electrodeU1mA drifting down against the commissioning value, leakage rising, one warm unit among cool ones on thermal imagingRepeat the electrical tests against the commissioning baseline before condemning the string
Pollution, mechanical damage and installation errorEroded or tracked sheds, a crack at the flange, a bent or sheared terminal, a missing or corroded earth boltExternal flashover marks with no internal damage; creepage short of the site pollution level; damage traced to transport or liftingCorrect the selection or the handling, then re-test the units that remain in service

Read the table as a triage order, not a diagnosis. One reading rarely proves a cause; the pattern across teardown, electrical test and service history does.

Failure Mode 1: Moisture Ingress Through a Seal

Water reaches the block column through the few places that are meant to be sealed: the top cap, the base fitting, the interface on a screened separable body, or a cable-end cap left off in storage. Thermal cycling then pumps moist air in and out of the cavity, so a seal that passes a factory routine test can still admit water after two or three seasons of daily temperature swing.

Screened separable 12 kV surge arrester body in black polymer with grey insulated cap and earth braid

The photograph above shows a screened separable arrester body of the kind used on 12 kV cable systems, where the screened interface rather than the shed profile is the part that must stay dry. On this family the interface is also the part most often disturbed, because it is opened every time the cable is tested or re-terminated.

At teardown the evidence is usually obvious once the housing is opened: white or grey deposits along the block column, tracking marks that follow the surface rather than passing through the ceramic, corroded spring contacts, and the smell of a wet cavity. A housing split that begins at a shed root and runs longitudinally is the mechanical end point of the same process, because the internal pressure rises as the blocks heat.

In the field the sequence is consistent. Insulation resistance falls away from the value recorded at commissioning, the DC reference voltage measured at 1 mA drops, and the resistive component of leakage current rises. None of those readings is meaningful without a commissioning record to compare against, which is the practical argument for writing a per-serial test value into the handover documents.

  • Keep the sealing caps fitted until the moment of connection, and refit them if the cable is tested after the arrester is installed.
  • Torque the top cap and the earth stud to the drawing; a cap tightened by feel is the most common source of a leak that appears in year two.
  • Store upright, indoors, and never lift a unit by its shed column or by the lead.

Failure Mode 2: Continuous Power-Frequency Overvoltage

An arrester that is asked to hold more voltage than its continuous operating voltage allows will not fail at once. It heats, its blocks degrade faster than the design allows, and it eventually fails thermally. The signature is that the damage is uniform: every block in the column shows the same overheating, which is how this cause is separated from a lightning event that damages one point.

Three situations produce it in distribution work. A single-phase earth fault on a system with an isolated or impedance-earthed neutral raises the healthy-phase voltage to phase-to-phase level for as long as the fault is allowed to persist, which on an isolated system can be hours rather than seconds. A ferroresonant condition, typically an unloaded transformer fed through a long cable or a set of single-pole switches, produces a sustained overvoltage that no arrester rating is designed to absorb. And a unit selected on the nominal system voltage rather than on the real maximum continuous phase-to-earth voltage will be under-rated for the site from the day it is installed.

This is why the rated voltage in the catalogue is not the selection figure. The continuous operating voltage has to cover the highest phase-to-earth voltage the system can present for an indefinite period, and the rated voltage has to cover a specified overvoltage for a specified time. The published values for three units in the current range show how far apart the two numbers sit.

ModelRated voltageContinuous operating voltageResidual at 8/20 µsResidual at 30/60 µs
YH5WZ-51/13451 kV40.8 kV≤134 kV≤114 kV
YH5WX-54/15054 kV43.2 kV≤150 kV≤128 kV
YH1.5W-30/80 (neutral)30 kV24 kV≤80 kV≤67.5 kV

The gap between the two columns is the margin the unit has for an earth fault. If the system is operated with one phase earthed for longer than the arrester's overvoltage capability allows, the margin is spent. Specifying the earthing arrangement, and the fault clearance time that actually applies, is more useful than adding a voltage class "for safety". Where the selection itself is still open, the working order for choosing an arrester for a 10 to 35 kV network covers the same inputs one by one.

Failure Mode 3: Energy Beyond the Class Rating

Every arrester is tested for a nominal discharge current at 8/20 µs, a high current at 4/10 µs, and a long-duration current at 2000 µs. Those three numbers, not the residual voltage alone, decide whether the unit survives the site. The stations and lines that fail arresters are usually the ones where the site duty was never translated into a class.

Polymer-housed station-type surge arrester with a multi-shed silicone column on a galvanised base bracket

The station-type unit above, with its multi-shed polymer column on a galvanised base bracket, is the shape in which that duty is highest: a single column carries the whole discharge, so a class that is one step short shows up here first.

Teardown evidence for an energy event is local, not uniform. Look for a single puncture through one block, a small cluster of fragmented blocks, metal spray confined to a few square centimetres, and a radial split in the housing. A unit that failed from overvoltage and a unit that failed from energy can look equally destroyed from the outside, which is why the location of the damage inside matters.

Two installation choices feed this failure mode without being the arrester's fault. Long phase and earth leads raise the voltage the arrester sees and lengthen the current path, and an arrester placed at the end of a run rather than at the equipment terminals leaves the equipment exposed to the first part of the surge. Both are corrected by moving the unit, not by buying a larger class. On exposed overhead lines the answer is usually a composite line arrester installed at the pole rather than a bigger station unit at the substation.

Failure Mode 4: Varistor Ageing and Thermal Runaway

Ageing is the mode with no external sign, which makes it the one that most often ends in a fire rather than a flashover. The blocks lose part of their nonlinearity over years of voltage and thermal stress, the resistive leakage current rises, the unit runs hotter, and the extra heat accelerates the process until the housing cannot contain it.

Because there is nothing to see, the only reliable evidence is a trend against a starting point. A DC reference voltage measured at 1 mA at commissioning, recorded per serial number, turns a routine test into a comparison. A drop of a few per cent from that value, repeated on the next visit, matters far more than the absolute figure, because the absolute figure depends on the block volume and cannot be borrowed from another site.

Thermal imaging under load is the other half of the check. A unit noticeably warmer than its neighbours in the same bay, at the same current, is a candidate for replacement even when its electrical readings have not yet moved. A surge counter tells you that discharges have occurred, not how much life they consumed, and what a surge counter does and does not record is worth reading before a counter value is used to condemn a unit.

Failure Mode 5: Pollution, Mechanical Damage and Installation Error

The last group is decided before the unit is ever energised: creepage selected for the wrong pollution level, a shed profile that traps water and dust, a polymer housing cracked in transport, a terminal bent while the phase lead was pulled into place, or an earth bolt left loose. All of them produce failures that look like arrester failures and are not.

Two linemen on a pole platform hoisting a distribution transformer with arresters fitted above the tank

The pole-top installation above is where the mechanical and installation causes are set: the arrester position relative to the transformer, the length of the earth run, and whether the unit is bolted to a bracket that flexes. A unit hanging on a bracket that moves will crack at the flange long before its blocks age.

Pollution failure shows as erosion and tracking on the sheds and as external flashover marks with a clean interior. The selection input is the site pollution level, not the voltage class, and the required creepage follows from it. Standard products are rated for a moderate or lighter soiling environment, +40 °C ambient, −40 °C low temperature, 3000 m altitude and a 35 m/s wind; a coastal, industrial or desert site that exceeds any of those needs to be stated at the enquiry, because the standard unit is not built for it.

The earth bond belongs in this group too. A corroded strap or a loose bolt adds resistance and inductance in the discharge path, and it fails inspection even when the arrester is sound. The earth bond at the arrester base and the route to the equipment earth should be checked with the same attention as the phase connection, and recorded in the same drawing.

What Does a Ruptured Arrester Change About Safe Working Distance?

A ruptured arrester is an energy release, not a failed component, and the distance that matters afterwards is a project figure rather than a single international number. Design practice relies on pressure-relief behaviour: a unit built to vent through a defined path splits in a controlled way instead of fragmenting, and IEC 60099-4 is where that behaviour and the associated test are specified.

Three distances are worth separating in the operating procedure. The first is the normal approach distance for live work, which comes from the local clearance rule for the voltage and is not an arrester property. The second is the exclusion zone after a rupture, which should be taken from the manufacturer's instruction for the specific design and from the pressure-relief test report, and which the supplier should be able to state in writing for the unit being quoted. The third is the handling distance at replacement, where the risk is a housing that splits as it is unbolted.

The practical rules are simple. Do not re-energise a bay whose arrester has ruptured, and do not test the unit in place to "confirm" the failure: the housing has already been loaded once. Isolate, replace, and test the units that shared the event before the circuit is returned to service. If a supplier cannot state the post-rupture clearance for the design in writing, that is a gap in the offer, not a detail to settle later.

Replace One Unit or the Whole Batch?

The question that follows every failure is whether the rest of the string is a spare-part problem or a batch problem. The answer comes from three inputs: whether the cause was external and local, whether the units share a production batch and a service history, and whether the tests on the survivors have moved together or stayed flat.

SituationReplace one unitReplace the batchReason
One rupture after a recorded storm, survivors at their commissioning U1mAYesNoThe cause was energy at one point, and the others did not absorb it
Two or more failures in the same bay or string within one seasonNoYesA shared duty or a shared batch is more likely than two independent events
U1mA drifting in the same direction on every unit testedNoYesAgeing is proceeding at the same rate across the batch
Visible shed erosion across all units at a coastal or industrial siteNoYesThe creepage selection is wrong for the site, so replacements of the same class will fail the same way
One failure after a cable test or a repair, other units not yet testedYes, then testOnly if tests show driftThe event was local, but the survivors still owe you a reading
High counter readings, all electrical tests within the commissioning valuesNoNoCounted discharges are not consumed life; keep monitoring

Where the batch decision is taken, replace with the same voltage class and the same connection arrangement, and correct the selection input that caused the failure at the same time. Replacing a batch of under-rated units with the same under-rated units is the most expensive way to repeat the fault.

What to Write Into the RFQ and the Datasheet

A specification that lists only the system voltage will be answered with a catalogue number, and the four inputs that decide whether the unit survives its site will be missing. State these as requirements:

  • System data: nominal voltage, highest system voltage, earthing arrangement (effectively earthed, impedance earthed or isolated neutral) and the earth-fault clearance time that actually applies.
  • Duty: continuous operating voltage, rated voltage, nominal discharge current, long-duration current at 2000 µs, high current at 4/10 µs, and the residual voltage at the discharge currents you are coordinating against.
  • Environment: pollution level and required creepage, ambient range, altitude, wind loading and any corrosive or coastal exposure, with the mounting position.
  • Construction: housing material and shed profile, mounting type (station bracket, pole, drop-out, screened separable), terminal and earth stud arrangement, and the pressure-relief behaviour in writing.
  • Documents: type test report to IEC 60099-4, routine test report per unit, approval drawing showing the earth bond and the clearance, and the measured DC reference voltage recorded per serial number.
  • Packing: sealed caps fitted, units crated upright, and the storage condition stated for the period before energisation.

For overhead insulated conductors the fitting type changes the specification rather than the rating: a piercing-type external gap arrester is specified by conductor size and by the series gap it forms, and a drop-out arrester by the disconnector behaviour that isolates a failed unit. Getting the fitting right is a separate decision from getting the class right, and both belong on the datasheet.

Where Nahu Group Fits

Nahu Group manufactures polymer-housed metal-oxide surge arresters from 3 kV to 220 kV, covering station, distribution, drop-out and piercing designs. The lightning arrester includes the YH and HY composite series for station and distribution mounting, the YH5WS-TB drop-out arrester for pole-top use, and the piercing-type external gap arrester for insulated overhead conductors.

To get a configuration, send the system nominal and highest voltage, the earthing arrangement and earth-fault duration, the equipment being protected with its insulation level, the mounting position, the site pollution level and the ambient range. With those, the rated voltage, the continuous operating voltage and the residual voltage class can be confirmed against the drawing before the order is placed. If the enquiry is a replacement after a failure, include the teardown photographs and the readings taken before the unit was removed.

Frequently Asked Questions About Surge Arrester Failure

What are the most common causes of surge arrester failure?

Moisture ingress through a seal, sustained power-frequency overvoltage, discharge energy beyond the class rating, varistor ageing and pollution or mechanical damage account for most failures. Moisture and ageing produce similar electrical readings, so the teardown decides between them. Energy events leave localised damage inside the column, which is the quickest way to rule the other causes out.

How can I tell whether an arrester failed from lightning or from moisture?

Look at where the damage sits. An energy event damages one block or a small cluster, sprays metal over a small area and splits the housing radially. Moisture tracks along the surface of the column and corrodes the contacts, and the housing splits longitudinally from a shed root. If the column is uniformly overheated, the cause is overvoltage rather than either of them.

What is U1mA and what change actually matters?

U1mA is the DC voltage at which the arrester passes 1 mA, the reference point defined for metal-oxide arresters without gaps. What matters is the change from the value recorded for that serial at commissioning: a few per cent in one direction, repeated on the next test, is a trend. An absolute figure taken from another site or another model tells you very little.

Can a surge arrester fail with no external sign?

Yes. Ageing and incipient moisture ingress both develop inside the housing, and the unit can look normal up to the point of thermal runaway. That is why the electrical readings and thermal imaging carry the weight in a maintenance programme, and why the commissioning record matters more than any single measurement taken later.

Is a high surge counter reading a reason to replace the arrester?

Not on its own. A counter records that discharges above its threshold occurred; it does not measure how much of the blocks' capability was used. A high count with stable electrical readings is a reason to shorten the test interval, not to replace. A low count with falling U1mA is the more serious combination.

Should every arrester on a pole be replaced when one fails?

Only when the evidence is shared. If one unit ruptured in a recorded storm and the others still read at their commissioning values, replace the failed unit. If two have failed within a season, or the survivors show the same U1mA drift or the same shed erosion, the batch is the problem and piecemeal replacement just moves the next failure forward.

Published Nov 24, 2026 · Nahu Group (NAHU Electric Technology)